Exposure rack
5°
Roof of a 4-floor building located in a centre of an industrial town (oil refinery, chemical industry) with 10,000 inhabitants
ISO 9223 - Measurement period: 2020-02-01 - 2021-02-01 Measuring inputed: 2022/08/23 | Steel | Zinc | Copper | Aluminium |
---|---|---|---|---|
ISO 9223 - Corrosion rate [g/m² year] | 41.4 | 2 | 5 | 0.1 |
Corrosivity category | C2 | C2 | C2 | C1 |
ISO 9223 - Standard deviation of corrosion rate [g/m² year] | ±0.7 | ±0.1 | ±0.6 | ±0.1 |
ISO 9223 - Measurement period: 2019-01-16 - 2020-01-27 Measuring inputed: 2023/08/04 | Steel | Zinc | Copper | Aluminium |
---|---|---|---|---|
ISO 9223 - Corrosion rate [g/m² year] | 32.3 | 4.1 | 8.1 | 0.2 |
Corrosivity category | C2 | C2 | C3 | C2 |
ISO 9223 - Standard deviation of corrosion rate [g/m² year] | ±48 | ±0.2 | ±0.3 | ±0.1 |
ISO 9223 - Measurement period: 2018-01-16 - 2019-01-16 Measuring inputed: 2023/08/04 | Steel | Zinc | Copper | Aluminium |
---|---|---|---|---|
ISO 9223 - Corrosion rate [g/m² year] | 19.2 | 3 | 5.3 | - |
Corrosivity category | C2 | C2 | C3 | - |
ISO 9223 - Standard deviation of corrosion rate [g/m² year] | ±1.4 | ±1.1 | ±0 | - |
Parameter | Value | Measurment period | |
---|---|---|---|
Rainfall [mm/year] | 581 | 2020-02-01 - 2021-02-01 | |
Temperature [°C] | 11.4 | 2020-02-01 - 2021-02-01 | |
SO2 [µg/m³] | 5 | P0 | 2020-02-01 - 2021-02-01 |
NOx [µg/m³] | 16 | 2020-02-01 - 2021-02-01 | |
Chloride deposition [mg/m² day] | 0.7 | S0 | 2020-02-01 - 2021-02-01 |
pH of rain | 5.2 | 2020-02-01 - 2021-02-01 | |
Relative humidity [%] | 73 | 2020-02-01 - 2021-02-01 | |
Time of wetness [%] | 42 | τ4 | 2020-02-01 - 2021-02-01 |
Exposure under shelter
University of Chemistry and Technology Prague, Technopark Kralupy, Nám. G. Karse 7, 278 01 Kralupy nad Vltavou, Czech Republic
Tomáš Prošek, prosekt@vscht.cz, +420 723 242 413
prosekt@vscht.cz