Site name:

AT, Linz

Country:

Austria

Atmosphere:

Industrial

Available space [m²]:

>50

Altitude [m]:

257

Operational since:

2015

This site is embedded in the St. Peter industrial area of Linz with voestalpine Stahl Linz steel mill as leading company. It consists of two separate fields. Field 1 is committed to accelerated, high salinity experiments (e.g.” VDA 621-414 – like”) and individual adapted exposure methods. Field 2, separated several meters from Nr.1 to avoid any cross contamination, is dedicated to classical atmospheric exposure. Being completely fenced and locating within the secured limits of the steel mill all fields are well protected against unauthorized influences and persons. Due to the vicinity of railroad tracks there are typical particle depositions (brake dust) present.

Address: Voestalpine Strasse 3, 4020 Linz, Austria
Corrosion category (ISO 9223)
ISO 9223 - Measurement period: 2015-01-01 - 2019-01-01
Measuring inputed: 2022/08/23
SteelZincCopperAluminium
ISO 9223 - Corrosion rate [g/m² year]10611.48.20.3
Corrosivity categoryC2C3C3C2
ISO 9223 - Standard deviation of corrosion rate [g/m² year]----
Environmental parameters
Parameter Value   Measurment period
Rainfall [mm/year]735 2015-01-01 - 2019-12-01
Temperature [°C]11.9 2015-01-01 - 2019-12-01
SO2 [µg/m³]13P1NaN - NaN
Chloride deposition [mg/m² day]3.3S1NaN - NaN
Relative humidity [%]70 2015-01-01 - 2019-12-01
Time of wetness [%]41τ42015-01-01 - 2019-12-01
Exposure racks
check_box
Exposure rack
check_box
Exposure rack
45°
check_box
Exposure rack
90°
check_box
Exposure rack
Customized

0° sheltered (VDA 621-414) and non-sheltered

Additional information

All relevant racks are orientated in north/south direction and shadow because of trees, other racks, etc. is avoided to fulfil the standards.

Contacts

voestalpine Stahl Linz, R&D dept. CTE

Gerald Luckeneder, gerald.luckeneder@voestalpine.com
gerald.luckeneder@voestalpine.com